FIELD: wood-working industry. SUBSTANCE: wood chip and polyethylene particles are intermixed, and the mixture is poured into the forming cradle mounted on a pallet. The pressing of sheet materials is carried out with the simultaneous formation of mutually connected spatial members at the temperature of 120-160 C, at the unit pressure of 2.0-2.5 MPa. The pressing time is 1 min per 1 mm of thickness. The articles are cooled up to the temperature of 20-40 C at the unit pressure of 0.5-1.0 MPa. EFFECT: enhanced efficiency. 10 cl, 3 dwg
Authors
Dates
1995-07-09—Published
1992-11-25—Filed